ABSTRACT:

FIELD OF USE
This invention relates to techniques for sealing flat-panel devices such as flat-panel displays.
BACKGROUND ART
A flat-panel device typically contains two generally flat plates positioned opposite each other. A flat-panel display is a type of flat-panel device utilized for displaying information. The two plates in a flat-panel display are commonly termed the faceplate and backplate. The faceplate, which provides the display's viewing surface, is part of a faceplate structure containing one or more layers or regions formed over the faceplate. The backplate is similarly part of a backplate structure containing one or more layers or regions formed over the backplate. The two plate structures are sealed together, typically through an outer wall, to form a sealed enclosure.
A flat-panel display utilizes mechanisms such as cathode rays (electrons), plasmas, and liquid crystals to display information on the faceplate. Flat-panel displays which employ these three mechanisms are generally referred to as cathode-ray tube (“CRT”) displays, plasma displays, and liquid-crystal displays. The constituency and arrangement of the display's two plate structures depend on the type of mechanism utilized to display information on the faceplate.
In a flat-panel CRT display, electron-emissive elements are typically provided over the backplate. Light-emissive elements are situated over the faceplate. When the electron-emissive elements are appropriately excited, they emit electrons that strike the light-emissive elements causing them to emit light visible on the faceplate. By appropriately controlling the electron flow from the backplate structure to the faceplate structure, a suitable image is displayed on the faceplate. The electron flow needs to occur in a highly evacuated environment for the CRT display to operate properly and to avoid rapid degradation in performance. It is thus critical to hermetically seal a flat-panel CRT display.
FIGS. 1
a
-
1
c
(collectively “FIG.
1
”) illustrate a conventional technique for sealing a flat-panel CRT display of the field-emission type, often referred to simply as a field-emission display (“FED”). The components of the FED being sealed in
FIG. 1
include backplate structure
10
, faceplate structure
12
, outer wall
14
, and multiple spacer walls
16
situated between plates structures
10
and
12
for preventing outside forces, such as air pressure, from collapsing or otherwise damaging the FED.
At the point shown in
FIG. 1
a
, spacer walls
16
are mounted on faceplate structure
12
, and outer wall
14
is connected to faceplate structure
12
through frit (sealing glass)
18
provided along the faceplate edge of outer wall
14
. Frit
20
is situated along the backplate edge of outer wall
14
. A pump-out tube (not shown) is typically affixed to backplate structure
10
for later evacuating the sealed FED. Prior to the sealing operation, backplate structure
10
is physically separate from the composite structure formed with faceplate structure
12
, outer wall
14
, and spacer walls
16
.
Structures
10
and
12
/
14
/
16
are placed in an alignment system
22
, aligned to each other, and brought into physical contact along frit
20
as shown in
FIG. 1
b
. Alignment system
22
is located in, or is placed in, an oven
24
. After being aligned and brought into contact along frit
20
, structures
10
and
12
/
14
/
16
are slowly heated in air to a sealing temperature ranging from 450° C. to greater than 600° C. Frit
20
melts. The FED is subsequently cooled down to room temperature. As frit
20
cools down, it seals composite structure
12
/
14
/
16
to backplate structure
10
.
At or near the end of the cooldown, the FED is removed from alignment system
22
and oven
24
. The pressure in the interior of the FED is brought down to the desired vacuum level by removing air through the pump-out tube. The pump-out tube is then closed. Aside from the pump-out tube,
FIG. 1
c
depicts the final hermetically sealed FED.
During the sealing operation, the upper edge of outer wall
14
, including frit
18
and frit
20
, is initially slightly higher than the upper edges of spacer walls
16
. As frit
20
melts, it compresses somewhat in the direction, commonly referred to as the z direction, perpendicular to plate structures
10
and
12
until spacer walls
16
meet backplate structure
10
. Frit
18
may also compress in the z direction during the sealing operation. Hence, plates structures
10
and
12
move relative to each other in the z direction as the FED is being sealed. A similar type of z motion would occur if a rectangular ring of frit were substituted for composite outer wall
14
/
18
/
20
.
A side effect of motion in the z direction is that faceplate structure
12
sometimes moves relative to backplate structure
10
in a direction perpendicular to the z direction. Hence, the alignment of plate structures
10
and
12
is sometimes degraded as a result of the z motion of structures
10
and
12
. Due primarily to differences in the coefficients of thermal expansion of plate structures
10
and
12
and alignment system
22
, the degradation in alignment can occur despite the use of system
22
. It would be desirable to hermetically seal a flat-panel display, especially a flat-panel CRT display such as an FED, according to a technique that largely avoids z motion between the displays two plate structures and thus avoids alignment degradation due to such z motion.
As frit
20
melts and compresses in the z direction, frit
20
normally spreads laterally over faceplate structure
12
. The lateral area of structure
12
can be increased in the peripheral area outside the viewing area to allow for frit
20
to spread laterally. However, it is typically desirable that the peripheral display area be as small a fraction as possible of the total lateral area of structure
12
. Accordingly, increasing the lateral area of structure
12
to allow room for frit
20
to spread is disadvantageous.
In addition, frit
20
may occasionally spread laterally beyond the normal area allocated for the spreading of frit
20
and damage components of the FED. A similar disadvantage would occur if composite outer wall
14
/
18
/
20
were replaced with a ring, again rectangular, of frit. In sealing two plate structures of a flat-panel display, especially a flat-panel CRT display such as an FED, together through a sealing structure, it would be desirable to have a technique for suitably restricting lateral spreading of the sealing material in the sealing structure.
PCT Patent Publication WO 98/26440 discloses a local-energy gap-jumping technique for sealing the backplate structure and faceplate structure of a flat-panel display. A rectangular frame of sealing material, typically frit, is sealed to the faceplate structure. The sealing frame laterally surrounds a group of spacer walls that extend further away from the faceplate structure than does the sealing frame. The backplate structure is placed vertically above the faceplate structure so that the sealing frame and spacer walls are situated between the two plate structures. The backplate structure lies directly on the spacer walls. Because the spacer walls are taller than the sealing frame at this point, a gap is present between the backplate structure and the sealing frame.
The two plate structures in PCT Patent Publication WO 98/26440 are held in a desired alignment using a suitable tacking mechanism. Energy is then transferred locally to portions of the sealing frame close to the backplate structure. The local energy, typically light energy provided from a laser or focused lamp, causes the sealing material to jump the backplate-structure-to-sealing-frame gap and hermetically seal the plate structures together.
By using spacer walls that are initially taller than the sealing frame, the sealing technique of PCT Patent Publication WO 98/26440 largely avoids undesired z motion during the sealing operation. However, utilization of a laser, focused lamp, or other local-energy producing mechanism

LandOfFree

Say what you really think

Search LandOfFree.com for the USA inventors and patents. Rate them and share your experience with other people.

Rating

Sealing of flat-panel device does not yet have a rating. At this time, there are no reviews or comments for this patent.

If you have personal experience with Sealing of flat-panel device, we encourage you to share that experience with our LandOfFree.com community. Your opinion is very important and Sealing of flat-panel device will most certainly appreciate the feedback.

Rate now

     

Profile ID: LFUS-PAI-O-3240830

  Search
All data on this website is collected from public sources. Our data reflects the most accurate information available at the time of publication.